自動焊接設備焊出來發黑是什么原因

來源:http://m.xihagames.com/  發布時間:2022-12-03 瀏覽次數:0

自動焊接設備的焊點焊道一般是白亮的,不過如果使用方法不正確的話,也可能導致焊出來發黑,如果自動焊接設備焊出來是黑的,可能原因有:
The weld bead of the automatic welding equipment is generally white and bright. However, if the use method is incorrect, it may also lead to black after welding. If the automatic welding equipment is black after welding, the possible reasons are:
1、氬氣沒有打開或者氣罐內已經沒有氬氣,需要檢查氬氣瓶閥門和氬氣表開關。
1. If the argon is not opened or there is no argon in the gas tank, check the valve of the argon cylinder and the switch of the argon meter.
2、鎢針露出陶瓷嘴距離太長,在焊接過程中氬氣并沒有起到防氧化作用。
2. The distance between the tungsten needle and the ceramic nozzle is too long, so argon does not play an anti oxidation role in the welding process.
3、自動焊接設備的參數調節過大,沒有按照工況調節相應的材料及厚度所應設置的電流大小及放弧時間。
3. The parameter adjustment of automatic welding equipment is too large, and the current size and arcing time that should be set for the corresponding material and thickness are not adjusted according to the working conditions.
4、工件表面雜質過多,沒有提前清理工件表面的油污、氧化物等雜質。
4. There are too many impurities on the surface of the workpiece, and the impurities such as oil and oxide on the surface of the workpiece are not cleaned in advance.
5、工件工藝要求過高,該型號的自動焊接設備配置不足,無法完成焊接需求。
5. Workpiece process requirements are too high, and the automatic welding equipment of this model is insufficient to meet the welding requirements.
山東自動焊接設備
怎么操作不發黑?
How to operate without blackening?
1、選擇符合工件加工需求的山東自動焊接設備配置,并根據弓箭情況調節好相應的參數。
1. Select the automatic welding equipment configuration that meets the workpiece processing requirements, and adjust the corresponding parameters according to the bow and arrow conditions.
2、在焊接的時候,要選擇合適的焊絲,所填焊絲直徑好小于工件厚度。
2. When welding, select the appropriate welding wire, and the diameter of the filled welding wire is better than the thickness of the workpiece.
3、焊接時,應盡量減小工件之間的焊縫距離,焊縫盡量清理干凈。
3. During welding, the weld distance between workpieces shall be minimized and the weld shall be cleaned as much as possible.
4、焊接到末端后停留一秒左右,千萬別立刻移開焊槍,防止后焊點氧化。
4. Stay for about one second after welding to the end. Never remove the welding gun immediately to prevent oxidation of the rear welding spot.
自動焊接設備焊出來發黑是什么原因已經講解完畢了,當然處理措施我們也列出來了,給您好的參考信息。更多相關事項就來我們網站http://m.xihagames.com咨詢吧!
The reason why the automatic welding equipment blackens after welding has been explained. Of course, we have also listed the treatment measures for your reference. Come to our website for more information http://m.xihagames.com Consult!

上一篇:數控焊接設備的日常三大檢查使用
下一篇:結構可以了解到焊接專機的注意事項

主站蜘蛛池模板: 欧美在线网址| 九九热在线观看| 99视频这里有精品| 亚洲精品成人在线| 综综综综合网| 在线观看不卡视频| 亚洲天堂免费在线视频| 亚洲国产福利| 亚洲六月丁香缴情久久丫| 先锋影音资源av| 午夜看片网站| 先锋影音va中文资源| 先锋影音资源av| 亚洲经典一区二区三区| 亚洲精品免费观看| 亚洲欧洲在线观看| 一级片www| 在线精品免费视频| 中文字幕在线视频第一页| 在线精品国产| 国产精品成人在线播放| 亚洲欧美成人综合| 亚洲haose在线观看| 97毛片| 国产手机精品视频| 国产手机在线小视频免费观看| 国产成人a∨麻豆精品| 国产欧美成人免费观看| 国产在线视频网址| 久久伊人精品青青草原高清| 毛片基地免费视频a| 欧美日韩网站| 思思在线精品| 亚洲天堂网视频| 重口人妖系列在线观看| 精品午夜久久影视| www.色五月.com| 国产无遮挡色视频免费视频| 精品久久久久久久久久久| 免费jjzz在在线播放国产成人| 欧美在线亚洲|